Renewable Energy

Emulsion-buffered screen limits printing damage in copper-plated HJT cells

A screen pattern with 4.7% emulsion coverage held minority-carrier lifetime degradation to 0.41% after 10,000 print cycles in copper-plated HJT cells.

Mira KovalenkoNovember 15, 20265 min read7 views
A woven printing mesh with a partially patterned emulsion coating held above a dark silicon wafer, illustrating the buffer-layer approach to reducing mesh contact damage.

Screen printing remains the standard way to deposit patterning layers on solar cells, but on copper-plated silicon heterojunction (HJT) devices the process carries a hidden cost: the mechanical pressure of each printing cycle progressively damages the cell's sensitive passivating contacts. Researchers in China have now identified the dominant wear mechanism and demonstrated a screen-design change that sharply limits the loss.

HJT cells depend on thin passivating stacks at the amorphous silicon/crystalline silicon interface, and those layers are vulnerable to the pressure and thermal treatment involved in printing. Damage there raises recombination losses and pulls down conversion efficiency, a point that matters because copper plating is seen as a route to lower metallization cost and less dependence on silver.

The difference lies in how the photoresist layer is printed, corresponding author Lang Zhou explained. Screens for silver paste open only 2–5% of their total area, and an emulsion layer covers the rest so the mesh never touches the wafer. Full-area photoresist coating usually requires a screen without emulsion coverage to spread resist evenly across the whole wafer, so the mesh comes into direct and extensive contact with the wafer on every cycle.

Production data had already shown the consequence: conversion efficiency fell from 26.2% to 25.7% across 15,000 consecutive printing cycles, driven mainly by lower open-circuit voltage and fill factor, while short-circuit current density and electrical resistance stayed largely unchanged. Minority carrier lifetime degradation climbed from 0.61% with a new screen to 11.0% after 15,000 cycles.

Using three-dimensional confocal microscopy, the team traced the decline to gradual wear of the screen mesh knuckles. As the knuckles flatten, their contact area with the wafer grows and the mechanical stress placed on the passivation layers rises. Scanning electron microscopy revealed no visible surface scratches, but photoluminescence measurements recorded increased recombination, pointing to damage at the amorphous/crystalline silicon interface rather than to gross surface defects.

To break that contact, the researchers added an emulsion buffer layer to the screen and evaluated six patterns with emulsion coverage ratios between 2.9% and 16.6%. The results exposed a trade-off: more emulsion meant better mechanical protection but poorer photoresist distribution. A coverage ratio of 4.7% gave the best balance, holding lifetime degradation to 0.41% after 10,000 printing cycles while maintaining relatively good coating uniformity.

The improvement is attributed to the emulsion layer keeping the mesh off the wafer, which reduces cumulative mechanical damage to the passivation stack. “The findings demonstrate that a relatively simple modification to screen design can substantially mitigate printing-induced degradation, offering a practical approach to improving the manufacturing reliability of copper-plated HJT solar cells,” Zhou said.

The work, published in Solar Energy as “Screen-printing photoresist induced efficiency degradation and mitigation in Cu-plated SHJ solar cells,” lands as copper metallization attracts wider interest. In April 2026, researchers at China's Nankai University reported a silver-free HJT cell at 25.2% efficiency, using plasma-induced interface engineering and copper electroplating to address adhesion, contact resistance and stability at the ITO interface. Separately, scientists at Germany's Forschungszentrum Jülich reached 23.08% with a fully copper-metallized HJT cell, a relatively small penalty against its silver-metallized counterpart, while a design combining silver-copper paste on the front side with silver contacts on the rear reached 23.95%.